Report Number *******
October XX, 20XX
ANALYSIS OF AN IMPACT FRACTURED, WELDED STEERING ARM SPINDLE ASSEMBLY
| Report for: | Report by: |
************** ************** ************** ************** ************** |
METALLURGICAL TECHNOLOGIES, INC., P.A. 160 Bevan Drive Mooresville, NC 28115 704-663-5108 |
Sections:
SUMMARY:
A welded left front spindle/steering arm assembly that had fractured at the fillet weld joint between the steering arm and inner brake boss was received for analysis to determine the mode of failure. The intact right front spindle/steering arm was submitted for comparison. Results indicate the weld joint failure occurred due to application of a single impact load. Examination of the fractured weld surface revealed a combination of ductile and brittle overload (dimpled rupture and cleavage) fracture, all consistent with impact loading. There are no indications of progressive crack growth via fatigue.
The initiation site for the fracture was a pre-existing crater crack formed during welding. Crater cracks occur at high temperature as the weld metal solidifies at the end of a weld pass. Similar crater cracks were identified at other fillet weld joints on the spindle/steering arm unit as well as in the fillet weld joints of the submitted comparison right front spindle/steering arm unit.
The presence of a dendritic structure with heavy oxidation in the cracks indicates solidification cracking. The presence of nickel plating along the fracture surface of the comparison unit weld crack confirms the cracks were present prior to application of the plating.
Chemical analysis of the steering arm base metal identified it as being SAE 4140 low alloy steel. Microanalysis of the steering arm base metal and the weld filler metal identified the filler metal as being SAE 4140 low alloy steel or a similar grade. An initial weld pass on the comparison unit fillet joint was identified as a grade of austenitic stainless steel. This initial pass using a stainless steel filler was not noted in the weld joint of the failed unit.
Hardness measurements of the cross-sectioned failed weldment identified the weld metal hardness as 27 HRC. The weld heat affected zone (HAZ) hardness ranged from a high of 29 HRC to a low of 19 HRC in the base metal. The spindle was not in a heat treated condition (not austenitized, quenched and tempered), however had been post weld stress relieved.
ANALYSIS:
Two welded steel (left and right front) spindle/steering arm assemblies were received for analysis. The left spindle/steering arm had fractured along the fillet weld joint between the steering arm and inner brake boss. The right front spindle/steering arm was submitted for comparison. The fracture is suspected to be the result of a broadside impact from another vehicle during the xxxxxxxxx Race at xxxxxxxxxx.
Figure 1 is an overall view of the failed assembly in the as-received condition A closer view of the steering arm fracture surface is presented in Figure 2. The fracture is through the complete circumferential joint weld and across the adjacent steering arm. The weld fracture exhibits a pre-existing hot crack (crater crack) further magnified in Figure 3. The crack extends across the weld joint width and is located at the end of the welding pass. The surface of the crack is oxidized with a heavy accumulation of rust. Fracture of the weld joint initiated at the pre-existing crack, and then grew in the directions indicated by arrows in Figure 3.
The other weldments of the spindle and steering arm were also examined. Similar crater cracks were identified in the fillet weld joint of the outer brake boss and support arm (Figures 4 and 5). Examination of weldments of the comparison spindle/steering arm revealed similar crater cracks at the steering arm/inner brake boss fillet weld joint. An example is shown in Figures 6 and 7. (Crater cracks also were observed on the outer brake boss/support arm fillet weld joint.) The cracks are located where the welding process stopped.
The fracture area containing the pre-existing crater crack at the initiation site on the steering arm was cut off and prepared for further analyses. The fracture surface was ultrasonically cleaned with a water base detergent (Alconox) and subjected to magnified examination using a scanning electron microscope (SEM).
Figure 8 is a low magnification SEM photomicrograph of the pre-existing hot/crater crack area and the surrounding fractured weld surface. Different fracture surface sites have been mapped and are shown in detail at higher magnification in subsequent figures. Note the pre-existing crater crack was approximately 0.125 (1/8) inch deep.
Figures 9 and 10 are increasing magnification views of the crater crack fracture surface along the weld outer surface. The higher magnification view of Figure 10 reveals the fracture surface to be severely oxidized indicating it opened during high temperature welding.
Figures 11 and 12 are increasing magnification views of the crater/hot crack surface close to the inner brake boss machined slot (lower hot crack area in Figure 8). The surface exhibits a dendritic structure indicative of a hot solidification crack. A region of ductile overload is also present between this hot crack region and the rest of the crater crack. The ductile overload is the result of a change in fracture planes during the impact fracture.
Figures 13 and 14 are high magnification SEM photomicrographs of the weld fracture surface on each side of the crater crack. Both figures exhibit ductile overload fracture surfaces. No indications of fatigue failure were noted around the crack. Additional examination of the weld fracture surface revealed dimples, which are ductile overload features, confirming failure occurred due to overload and not fatigue.
Figures 15 and 16 are increasing magnifications of the transition region between the weld HAZ and the base metal. The fracture surface topography changes from ductile overload in the HAZ to cleavage in the base metal. The presence of cleavage in the base metal fracture surface is indicative of failure due to high impact loading and a pearlitic (non-quenched and tempered) microstructure.
The SEM examined fracture surface sample was cross-sectioned axially through the crater crack and prepared for metallographic examination in accordance with ASTM E3-01. The polished surface was micro-etched (2% Nital) to reveal the cross-sectioned microstructure. This was done as recommended by ASTM E407-99.
Figure 17 is a montage of two optical photomicrographs exhibiting the complete weldment fracture cross-section. The initiation site and crater/hot crack areas are identified.
Figures 18 and 19 are higher magnifications of the initiation site. Noted is the nickel-plating along the outer weld surface. No nickel plating is observed along the fracture surface suggesting the crater crack was closed at the surface or possibly filled by a thin oxide film during nickel plating.
Figure 20 is a high magnification view of oxidation lining the walls of voids in the weld metal. This also indicates a hot solidification crack.
Figure 21 is a high magnification photomicrograph of the steering arm microstructure away from the HAZ. The structure is primarily pearlite indicating that the base metal originally was in an annealed or normalized condition (not austenitized, quenched and tempered).
The effects of heat input during welding were investigated by microhardness testing across the weldment. A profile was generated of the weld/HAZ/base metal hardness by testing at fine increments across the weldment and into the steering arm base metal. The measurements were made using a Knoop (HK) indenter with a 300-gram load in accordance with ASTM E384-99є1 guidelines. The HK values were converted approximately to Rockwell "C" scale (HRC) using the appropriate formula in ASTM E140-02.
The generated profile is presented in Figure 22. The hardness of the weld metal was 27 HRC at the inner edge of the weld. Hardness of the HAZ metal varied from a high of 29 HRC to a low of 20 HRC. The base metal exhibited a hardness value of 19 HRC. A hardness of 20 HRC corresponds approximately to a tensile strength of 110 ksi. The hardness of the HAZ indicated the weldment was stress relieved and tempered after welding.
Chemical composition of the steering arm body was determined using an optical emission spectrometer (OES) in accordance with ASTM E415-99a. The analysis identified the metal as meeting the requirements of SAE 4140 low alloy steel (Table 1).
Due to sample size restrictions the weld filler metal was analyzed using the energy dispersive x-ray spectrometer (EDS), in conjunction with the SEM. The analysis was conducted in general accordance with ASTM E1508-98 (03). The results indicate the filler metal is a low alloy steel similar to SAE 4140. EDS spectra of the weld filler metal and the steering arm body are presented in Figures 23 and 24 respectively. The displayed spectra are almost identical.
A fillet weld from the comparison spindle/steering arm assembly that also had a crater crack present was axially cross-sectioned through the crack, metallographically prepared and micro-etched. Figure 25 is a montage of the cross-sectioned comparison fillet weld with a crater crack. This crater crack is approximately 0.08 inch deep, somewhat shallower than the 0.125 inch depth in the failed assembly. The initial weld pass (inner pass) does not etch and was made with a stainless steel filler metal. EDS analysis (Figure 26) identified it as a chromium-nickel (austenitic) stainless steel.
Figures 27 and 28 are increasing magnification views of the crater crack surfaces. Figure 28 shows that nickel-plating is present both on the outer weld surface and along both surfaces of the crater crack near the opening. The presence of nickel plating reveals that the crack had been formed and was open prior to the plating process.
Figures 29 and 30 are increasing magnification views of the weld crack tip and adjacent inter-dendritic solidification or "hot" cracks. A layer of oxidation lines the crack surfaces, which is further confirmation of hot - solidification cracking.
CONCLUSIONS:
Fracture of the steering arm/inner brake boss fillet weld was the result of a single impact load. Failure initiated along the weld, at a 1/8-inch deep crater crack that formed on cooling at the end of a weld pass. Similar cracks were noted at other fillet weld joints both on the failed unit and on a comparison unit.
The ductile and cleavage fracture surfaces (with no indications of progressive cracking via fatigue) identify impact overload as the mode of failure. The presence of a dendritic structure with oxidation in the crater crack and inter-dendritic cracks of the failed unit as well as nickel plating along the fracture surface of the comparison unit, confirms hot solidification cracking as the source of the failure initiation.
CHEMICAL ANALYSIS
TABLE I
Chemical Composition (wt. %)
| Element | Steering Arm |
SAE 4140 Specifications |
| Carbon | 0.39 |
0.38-0.43 |
| Manganese | 0.84 |
0.75-1.00 |
| Phosphorous | 0.013 |
0.030 max |
| Sulfur | 0.033 |
0.040 max |
| Silicon | 0.32 |
0.15-0.35 |
| Chromium | 0.87 |
0.80-1.10 |
| Molybdenum | 0.16 |
0.15-0.25 |
The steering arm meets the chemical composition requirements of SAE 4140
low alloy steel.
Depth (mils) |
Rockwell HRC |
Knoop HK |
-2 |
27 |
290 |
0 |
28 |
294 |
2 |
29 |
304 |
5 |
29 |
307 |
10 |
26 |
287 |
15 |
28 |
296 |
20 |
28 |
296 |
25 |
25 |
280 |
30 |
23 |
265 |
40 |
25 |
280 |
50 |
20 |
249 |
75 |
20 |
253 |
100 |
19 |
247 |
150 |
20 |
253 |
200 |
20 |
253 |